en kg / mmm |
E en Mpa |
G en Mpa |
en Mpa |
en Mpa |
en Mpa |
| METAUX |
aciers |
7800 |
205000 |
79000 |
400 à 1600 |
|
|
| aluminium AU4G |
2800 |
75000 |
29000 |
450 |
|
|
| titane TA 6V |
4400 |
105000 |
40300 |
1200 |
|
|
| cuivre |
8800 |
125000 |
48000 |
200 à 500 |
|
|
| nickel |
8900 |
220000 |
|
500 à 850 |
|
|
| beryllium |
1840 |
294000 |
|
200 |
|
|
| silice |
2200 |
95500 |
|
|
|
|
| RENFORTS nus |
verre R hautes performances |
2500 |
86000 |
|
3200 |
|
|
| verre E applications courantes |
2600 |
74000 |
30000 |
2500 |
|
|
| kevlar 49 |
1450 |
130000 |
12000 |
2900 |
|
|
| carbone HR haute résistance |
1750 |
230000 |
50000 |
3200 |
|
|
| carbone HM haut module |
1800 |
390000 |
20000 |
2500 |
|
|
| bore |
2600 |
400000 |
|
3400 |
|
|
| alumine |
3700 |
380000 |
|
1400 |
|
|
| silicate d’alumine |
2600 |
200000 |
|
3000 |
|
|
| carbure de silicium |
3450 |
450000 |
|
3000 |
|
|
| polyéthylène |
960 |
100000 |
|
3000 |
|
|
| RESINES |
époxy Ciba LY 5082/5083 |
1200 |
3050 |
1600 |
59 |
97 |
|
| phénolique |
1300 |
3000 |
1100 |
70 |
|
|
| polyester |
1200 |
4000 |
1400 |
80 |
|
|
| polycarbonate |
1200 |
2400 |
|
60 |
|
|
| vinylester |
1150 |
3300 |
|
75 |
|
|
| silicone |
1100 |
2200 |
|
35 |
|
|
| uréthane |
1100 |
700 à 7000 |
|
30 |
|
|
| polyamide |
1400 |
4000 à 19000 |
1100 |
70 |
|
|
| 60% fibre en volume |
UD verre |
2080 |
45000 |
4500 |
1250 |
600 |
63 |
| UD kevlar |
1350 |
85000 |
2100 |
1410 |
280 |
45 |
| UD carbone |
1530 |
134000 |
4200 |
1270 |
1130 |
63 |
| tissu équilibré verre 50% Vf |
1900 |
20000 |
2850 |
400 |
390 |
|
| tissu équilibré kevlar 50% Vf |
1330 |
22000 |
|
500 |
170 |
150 |
| tissu équilibré carbone 45% Vf |
1450 |
54000 |
4000 |
420 |
360 |
55 |
| AMES |
balsa |
150 |
3000 |
100 à 250 |
8 à 18 |
|
|
| CtP |
550 |
8000 |
|
|
|
|
| samba |
|
|
|
|
|
|
| mousse de polyuréthane |
30 à 70 |
25 à 60 |
20 |
|
|
|
| mousse de polystyrène |
30 à 45 |
20 à 30 |
10 |
0,25 à 1,25 |
|
|